by Luna Conradus September 11, 2026
The moment the kiln opens decides weeks of work. If the result isn't right, the cause almost never lies in the firing itself, but in something that happened before - a coat that wasn't dry, a fingerprint on the clay body, a bisque firing that was run too cool. The good news: the five most common defects have clear causes, and most pieces can be saved. This article matches each defect to its cause and tells you what to do about it.
What it looks like: Areas where the clay body is bare, while the glaze next to it has pulled together into a bead. The edges are rounded, not chipped - the glaze has literally retreated during the firing.
The causes: Almost always one of three. The glaze coat had not dried through before firing. The clay body was not free of dust and grease - a fingerprint is enough. Or the surface was so rough that the glaze could not grip evenly. A coat that is too thick also encourages crawling, because the drying layer shrinks and cracks.
What helps: Wipe the piece with a damp microfibre cloth before glazing and don't touch it with greasy fingers afterwards. Let each coat dry - the whole process is described in the article on applying glaze correctly. On a rough or heavily grogged clay body, apply the first coat thinned and work it into the texture with the brush - or dampen the piece beforehand so it takes up the glaze evenly.
What it looks like: Fine holes or crater-like dips in the melted glaze, sometimes in just one spot, sometimes spread across the whole surface.
The cause: Gases. The clay releases gas during the glaze firing - organic components break down, water of crystallisation escapes. As long as the glaze is fluid enough, the bubbles rise and the surface closes again. If the glaze solidifies too early or is too viscous, the craters remain.
What helps: The most effective lever is the bisque firing. Traditionally, bisque is fired between 850 and 900 °C; BOTZ recommends around 950 °C instead, because the clay is then largely degassed and releases nothing more in the second firing. Two further points: don't apply too thickly, and keep to the hold time - it gives the melt time to close up again. With heavily grogged clay, it helps to smooth the surface while throwing with a rib or rubber kidney.
What it looks like: Larger, burst bubbles, often with sharp edges - the coarser sibling of pinholes.
The causes: Usually a coat that is too thick, especially with flowing glazes. With the crackle glazes, applying on both sides causes blisters on some clays; BOTZ recommends a bisque firing at 1000 °C for these. A final temperature that is too high can also cause blisters, because glaze and clay then react with each other.
What helps: Reduce the coat thickness, glaze only the outside if in doubt, and check the actual kiln temperature. How to find out what really reaches your kiln chamber is explained in the article on the firing curve for the glaze firing.
Three of the five defects come down to the same thing: how the kiln fires. Pinholes form when the glaze solidifies before the gases are out. Blisters form when the firing is too hot. And running glaze is often simply the result of a temperature that is higher than displayed.

Two adjustments are therefore worth a second look before you doubt the glaze. The hold time gives the melt time to settle and close up risen bubbles - 10 to 20 minutes for earthenware, 10 to 30 in a stoneware firing. And the actual temperature in the kiln chamber, which can differ from the display: a kiln often fires hotter at the top than at the bottom, and the thermocouple only measures in one place.
What it looks like: Glaze on the kiln shelf, a thickened bead at the lower edge, in the worst case a piece that is fused to the shelf.
The causes: Three, and you can work through them in order. First: it is intentional - some glazes are meant to run and carry a drop pictogram for this. Second: the coat is too thick. Third: the temperature is too high. Even a correctly applied glaze will run if the kiln fires hotter than the controller shows.
What helps: Glaze the bottom third only thinly, wipe the foot generously clean and protect the kiln shelf with kiln wash 9010. On vertical surfaces, the tendency to run is naturally greater than on flat ones - a plate is more forgiving than a tall vase.
What it looks like: A network of hairline cracks in the surface, often only fully visible days after the firing.
The cause: Glaze and clay body contract by different amounts as they cool. If the glaze contracts more, it is under tension and cracks. This is not a question of firing, but of the combination of glaze and clay - the same glaze can stay smooth on a different clay.
What helps: If the network is unwanted, the only fix is a change - a different glaze or a different clay. If it is wanted, there are glazes built exactly for this; then it is called crackle and gets coloured. Both are explained in the article on crackle glazes. For tableware, the same applies in both cases: a crackled surface does not belong on the inside.
Not every flaw after firing is a glaze defect. Three belong to the clay body, and a second firing won't help with them.
Cracks in the clay. They form while drying or when joining two parts, often at handles and attachments. The cause is almost always uneven drying or a joint that was too dry. Prevention means: dry slowly and covered, score the joining surfaces and work with slip.
Burst hollow forms. A closed form without an air hole is a pressure chamber. The trapped air expands during firing and bursts the piece - usually taking its neighbours with it. Every closed form needs a small hole, pierced at the leather-hard stage.
Warped bases. In a high firing the clay body softens; large flat forms sag or warp. Even wall thicknesses help, and for long narrow pieces, a self-made kiln support that holds the form.
The most important sentence for anyone standing disappointed in front of the kiln: a failed piece is rarely lost. Bare spots, crawling and thin areas can be reglazed and fired again.
The method: fill the bare spots with glaze, let them dry thoroughly and then glaze over the whole piece once more with a soft brush so that no step remains. Then back into the kiln. Because an already fired glaze is a smooth, barely absorbent surface, it helps to apply the new coat rather thinly and in several passes.
What affects the clay body cannot be saved: cracks in the clay, burst hollow forms without an air hole, warped bases. Anything that only affects the glaze, on the other hand, is a case for a second firing.
A single failed firing is bad luck. The same defect in the third firing in a row is a pattern - and then it pays to search methodically instead of continuing to experiment.
The order in which causes can be ruled out is always the same: First the clay - is it the same as before, the same batch, the same grog content? Then the bisque firing - what temperature, what hold time? Then the glaze - stirred properly, right number of coats, dried enough? Finally the firing - final temperature, hold time, position in the kiln.
Because this only works if you write it down, a simple firing log is the most useful tool in the studio: date, clay, glaze, coats, temperature, hold time, result. After ten firings you will see patterns you would otherwise miss - for example that pieces at the bottom of the kiln consistently turn out differently from those at the top.
Not every flaw shows when the kiln is opened. Three appear with a delay - and are therefore often blamed on use rather than on making.
Cracks that keep growing. A crackle network can become denser over days and weeks, because the tension between glaze and clay body is released slowly. A piece that looked smooth after firing can be finely crazed a month later.
Moisture in the clay body. Low-fired ceramics absorb water when washed. If they then sit damp in the cupboard, this can show over time as stains or a musty smell. Handmade pottery is therefore washed by hand and dried in a well-ventilated place.
Frost damage. Garden ceramics made of clay that is not fired to density absorb water; when this water freezes, it bursts the clay body from the inside. Whether a piece is frost-proof is decided by the clay through its sintering point - not by the glaze on top.
Three habits prevent most defects before they happen: